Mechanical properties of titanium
1. The tensile strength of pure titanium is 265~353MPa, and that of general titanium alloys is 686~1176MPa, currently up to 1764MPa. Titanium alloys are as strong as many steels, but the specific strength of steel is far inferior to titanium alloys.
2. The compressive strength of titanium and titanium alloys is not less than its tensile strength. The compressive yield strength and tensile yield strength of industrial pure titanium are approximately equal, while the compressive strength of Ti-6AI-4V and Ti-5AI-2.5Sn is slightly higher than the tensile strength.
3. Shear strength is generally 60% to 70% of tensile strength. The compressive yield strength of titanium and titanium alloy sheets is approximately 1.2 to 2.0 times the tensile strength.
4. Under normal atmospheric atmosphere, the durability limit of processed and annealed titanium and titanium alloys is 0.5 to 0.65 tensile strength. When subjected to 10 million fatigue tests in the notched state (Kt=3.9), the endurance limit of annealed Ti-6AI-4V is 0.2 times the tensile strength.
5. The hardness of the highest purity grade of industrially pure titanium is usually less than 120HB (Brinnell hardness), and the hardness of other industrially pure titanium is 200 to 295HB. The hardness of pure titanium castings is 200~220HB. The hardness value of titanium alloy in the annealed state is 32~38HRC (Rockwell), which is equivalent to 298~349HB. The hardness of as-cast Ti-5Al-2.5Sn and Ti-6AI-4V is 320HB, and the hardness of low-gap impurity Ti-6Al-4V castings is 310HB.
6. The tensile elastic modulus of industrial pure titanium is 105~109GPa. The tensile elastic modulus of most titanium alloys in the annealed state is 110~120GPa. Age-hardened titanium alloys have a slightly higher tensile elastic modulus than in the annealed state, and the compressive elastic modulus is equal to or greater than the tensile elastic modulus. The specific elastic modulus of titanium alloy is equal to that of aluminum alloy, second only to beryllium, molybdenum and some high-temperature alloys.
7. The torsion or shear modulus of industrial pure titanium is 46GPa, and the shear modulus of titanium alloy is 43~51GPa. In order to improve the strength of titanium alloys, increasing the gap content will have harmful effects on the impact resistance and fracture toughness of the alloy. Depending on the type and state of the titanium alloy, the Charpy notch impact strength value of denatured industrial pure titanium is 15~54J/㎡, and it is about 4~10J/㎡ in the casting state. The impact strength of titanium alloy in the annealed state is 13~25.8J/㎡, and that in the aged state is slightly lower. The Charpy V-notch impact strength of Ti-5AI-2.5Sn in the cast state is 10J/㎡, and that of Ti-6AI-4V is 20~23J/㎡. The lower the oxygen content of titanium alloys, the higher this value.
8. Many titanium alloys have high fracture toughness, or in other words, titanium alloys have good resistance to crack propagation. Annealed Ti-6AI-4V is a material with excellent toughness. When the notch concentration coefficient Kt=25.4mm, the ratio of notched tensile strength to non-notched tensile strength is greater than 1.
9. Titanium alloys can maintain certain properties at high temperatures. Generally, industrial titanium alloys can maintain their properties at a temperature of 540°C, but they can only be used for a short time. The sufficient temperature range for a long time is 450~480°C. Titanium alloys have been developed for use at temperatures of 600°C. As a missile material, titanium alloy can be used at a temperature of 540℃ for a long time and at a temperature of 760℃ for a short time.
10. Titanium and titanium alloys can still maintain their original mechanical properties at low and ultra-low temperatures. As the temperature decreases, the strength of titanium and titanium alloys continues to increase, while the ductility gradually becomes worse. Many annealed titanium alloys also have sufficient ductility and fracture toughness at -195.5°C. Ti-5AI-2.5Sn, which contains extremely low interstitial elements, can be used at -252.7°C. The ratio of its notched tensile strength to non-notched tensile strength is 0.95~1.15 at -25.7°C.
Liquid oxygen, liquid hydrogen and liquid fluorine are important propellants in missiles and space devices. The low-temperature properties of materials used to make cryogenic gas containers and cryogenic structural parts are very important. When the microstructure is equiaxed and the content of interstitial elements (oxygen, helium, hydrogen, etc.) is very low, the ductility of titanium alloys is still above 5%. Most titanium alloys have poor ductility at -252.7°C, while the elongation of Ti-6AI-4V reaches 12%.
The above content is reproduced from Titanium House